序号 Test | A | B | C | D | a | b | c | d |
No. | 温度 Temp./℃ | 压力 Press/MPa | 时间 Time/min | 夹带剂 co-solvent content/mL | 纤维素 pulp yield/% | 半纤维素 Hemicellulose/% | 木质素 Lignin/% | 脱木质素率 Delignification yield/% |
0 | - | - | - | - | 53.40 | 18.67 | 27.03 | - |
1 | 160 | 16 | 30 | 1.5 | 44.89 | 19.29 | 8.29 | 69.32 |
2 | 160 | 20 | 60 | 2 | 52.11 | 10.84 | 8.67 | 67.90 |
3 | 160 | 24 | 90 | 2.5 | 53.26 | 16.54 | 7.71 | 71.47 |
4 | 180 | 16 | 60 | 2.5 | 50.52 | 15.71 | 6.46 | 76.09 |
5 | 180 | 20 | 90 | 1.5 | 50.87 | 18.54 | 5.25 | 80.59 |
6 | 180 | 24 | 30 | 2 | 45.10 | 18.35 | 6.66 | 75.35 |
7 | 200 | 16 | 90 | 2 | 52.42 | 17.67 | 6.23 | 76.96 |
8 | 200 | 20 | 30 | 2.5 | 52.58 | 15.34 | 6.26 | 76.83 |
9 | 200 | 24 | 60 | 1.5 | 46.78 | 20.95 | 5.18 | 80.84 |
Ka1 | 50.09 | 49.28 | 47.52 | 47.51 | 纤维素含量A3B2C3D3 |
| ||
Ka2 | 48.83 | 51.85 | 49.80 | 49.88 | ||||
Ka3 | 50.59 | 48.38 | 52.18 | 52.12 | ||||
Ra | 1.76 | 3.47 | 4.66 | 4.61 | ||||
Kb1 | 15.56 | 17.56 | 17.66 | 19.59 | 半纤维素含量A3B3C1D1 |
| ||
Kb2 | 17.53 | 14.91 | 15.83 | 15.62 | ||||
Kb3 | 17.99 | 18.61 | 17.58 | 15.86 | ||||
Rb | 2.43 | 3.7 | 1.83 | 3.73 | ||||
Kc1 | 8.22 | 6.99 | 7.07 | 6.24 | 木质素含量A3B3C3D1 |
| ||
Kc2 | 6.12 | 6.72 | 6.77 | 7.18 | ||||
Kc3 | 5.89 | 6.39 | 6.39 | 6.81 | ||||
Rc | 2.33 | 0.48 | 0.68 | 0.94 | ||||
Kd1 | 69.56 | 74.12 | 73.83 | 76.91 | 脱木质素率A3B3C3D1 |
| ||
Kd2 | 77.34 | 75.11 | 74.94 | 73.40 | ||||
Kd3 | 78.21 | 75.88 | 76.34 | 74.80 | ||||
Rd | 8.65 | 1.76 | 2.51 | 3.51 |