混合料

拌和温度/˚C

拌和速率/(r·min−1)

20

30

40

50

70#基质沥青

140

139.1

187.9

247.3

303.1

150

119.3

162.0

210.8

254.3

160

107.9

147.8

185.0

228.2

170

101.8

138.9

175.9

211.7

180

96.9

131.6

168.5

201.7

SBS改性沥青

140

160.8

218.5

279.6

350.3

150

142.8

193.5

252.6

309.3

160

131.0

174.1

222.3

279.2

170

113.2

161.3

204.5

238.0

180

105.8

148.7

184.1

217.9

橡胶沥青

140

165.0

231.1

299.1

360.3

150

145.7

208.1

266.1

317.3

160

137.3

186.1

241.2

292.1

170

124.5

165.8

212.0

260.6

180

115.7

151.1

192.6

235.8

Evotherm温拌沥青

140

116.9

167.1

216.5

254.6

150

103.1

146.8

187.8

223.2

160

99.1

136.4

169.5

209.9

170

95.3

127.3

163.1

199.9

180

91.8

122.8

155.6

191.4

ACMP1温拌沥青

140

109.2

153.0

193.2

242.7

150

100.4

138.3

174.3

220.2

160

96.0

130.8

165.3

206.9

170

91.1

123.8

156.4

196.0

180

86.3

122.9

153.2

186.5