沥青类型 | 掺量(%) | 135℃ | 165℃ | 拌合温度℃ | 压实温度℃ | 沥青类型 | 掺量(%) | 135℃ | 165℃ | 拌合温度℃ | 压实温度℃ | ||
炭 黑 改 性 沥 青 | 基质沥青 | - | 0.210 | 0.050 | 140.0~147.5 | 117.3~128.7 | 复 合 改 性 沥 青 | SBS 改性 沥青 | - | 0.591 | 0.193 | 164.8~167.8 | 155.8~160.3 |
热解炭黑改性沥青 | 5% | 0.256 | 0.052 | 144.9~150.7 | 127.2~136.0 | ||||||||
10% | 0.353 | 0.060 | 151.3~155.3 | 139.0~145.1 | |||||||||
15% | 0.442 | 0.117 | 158.6~162.3 | 147.5~153.1 | SBS~热解炭黑改性沥青 | 5% | 0.623 | 0.214 | 167.2~170.1 | 158.3~162.8 | |||
20% | 0.478 | 0.122 | 158.8~162.4 | 148.7~153.8 | 10% | 0.838 | 0.263 | 168.4~170.5 | 162.2~165.3 | ||||
25% | 0.491 | 0.127 | 160.3~163.7 | 150.4~155.4 | 15% | 0.912 | 0.342 | 173.0~175.1 | 166.7~169.8 | ||||
偶联PCB改性沥青 | 10% | 0.387 | 0.086 | 155.2~159.2 | 143.2~149.2 | 20% | 1.211 | 0.481 | 177.1~178.7 | 172.1~174.6 | |||
15% | 0.458 | 0.118 | 159.1~162.7 | 148.5~153.8 | 25% | 1.306 | 0.526 | 177.9~179.5 | 173.3~175.6 |